TRI Environmental, Inc. provided the following test results
UV Resistance (ASTM D 4355 – 500 hour exposure) Tensile Properties (ASTM D 5035/ECTC)
(4 inch wide strip specimen)
Baseline Properties | |
---|---|
MD – Maximum Load (ppi) | 14.6 |
TD – Maximum Load (ppi) | 18.7 |
MD – Elongation @ Max Load (%) | 19.3 |
TD – Elongation @ Max Load (%) | 27.7 |
Light Penetration (ECTC Guidelines) | |
---|---|
Baseline Reading | 125 |
Reading with sample | 10 |
% Light Penetration | <8 |
Swell (ECTC) | |
---|---|
Dry thickness (mils) | 1984 |
Thickness after soak (mils) | 2098 |
% change | 0 |
Water Absorption (ASTM D 1117/ECTC) | |
---|---|
Pre-soak Weight (grams) | 69 |
Post-Soak (grams) | 152 |
Weight change (grams) | 82 |
% Weight Change | 119 |
Sediment Control (ASTM D 5141) | |
---|---|
Test material: | Sand sieved thru No. 10 sieve |
Filtering Efficiency (%) | 40.8 |
Flow Rate (liter/minute) | 150 |
500 Hour Exposed Properties | |
---|---|
MD – Maximum Load (ppi) | 10.2 |
TD – Maximum Load (ppi) | 13.8 |
MD – Elongation @ Max Load (%) | 16.9 |
TD – Elongation @ Max Load (%) | 16.6 |
Resiliency (ASTM D 6524) | |
---|---|
Pre-loading thickness (mils) | 1943 |
Post-loading thickness (mils) | 326 |
% change | -83 |
Maximum Burn Distance (in) | |
---|---|
Mass/unit area (oz/sq. yd) | 50.89 |
Mass/unit area (g/sq. meter) | 1725 |
Smolder Resistance (ECTC) | |
---|---|
Maximum Burn Distance (in) | .29 |